Sintered SmCo Magnet Pwopriyete fizik | |||||||||
Materyèl | Klas | Remanans | Rev. Temp. - Coeff. Nan Br | Fòs kontrent | Intrinsèques fòs kontrent | Rev. Temp.-Coeff. Nan HCJ | Maks. Pwodwi enèji | Maks. Tanperati opere | Dansite |
Br (KGs) | Hcb (KOe) | Hcj (KOe) | (BH) max. (MGOe) | g / cm³ | |||||
SmCo5 | XG16 | 8.1-8.5 | -0.050 | 7.8-8.3 | 15-23 | -0.30 | 14-16 | 250 ℃ | 8.3 |
XG18 | 8.5-9.0 | -0.050 | 8.3-8.8 | 15-23 | -0.30 | 16-18 | 250 ℃ | 8.3 | |
XG20 | 9.0-9.4 | -0.050 | 8.5-9.1 | 15-23 | -0.30 | 19-21 | 250 ℃ | 8.3 | |
XG22 | 9.2-9.6 | -0.050 | 8.9-9.4 | 15-23 | -0.30 | 20-22 | 250 ℃ | 8.3 | |
XG24 | 9.6-10.0 | -0.050 | 9.2-9.7 | 15-23 | -0.30 | 22-24 | 250 ℃ | 8.3 | |
XG16S | 7.9-8.4 | -0.050 | 7.7-8.3 | ≥23 | -0,28 | 15-17 | 250 ℃ | 8.3 | |
XG18S | 8.4-8.9 | -0.050 | 8.1-8.7 | ≥23 | -0,28 | 17-19 | 250 ℃ | 8.3 | |
XG20S | 8.9-9.3 | -0.050 | 8.6-9.2 | ≥23 | -0,28 | 19-21 | 250 ℃ | 8.3 | |
XG22S | 9.2-9.6 | -0.050 | 8.9-9.5 | ≥23 | -0,28 | 21-23 | 250 ℃ | 8.3 | |
XG24S | 9.6-10.0 | -0.050 | 9.3-9.9 | ≥23 | -0,28 | 23-25 | 250 ℃ | 8.3 | |
Sm2Co17 | XG24H | 9.5-10.2 | -0.025 | 8.7-9.6 | ≥25 | -0.20 | 22-24 | 350 ℃ | 8.3 |
XG26H | 10.2-10.5 | -0.030 | 9.4-10.0 | ≥25 | -0.20 | 24-26 | 350 ℃ | 8.3 | |
XG28H | 10.3-10.8 | -0.035 | 9.5-10.2 | ≥25 | -0.20 | 26-28 | 350 ℃ | 8.3 | |
XG30H | 10.8-11.0 | -0.035 | 9.9-10.5 | ≥25 | -0.20 | 28-30 | 350 ℃ | 8.3 | |
XG32H | 11.0-11.3 | -0.035 | 10.2-10.8 | ≥25 | -0.20 | 29-32 | 350 ℃ | 8.3 | |
XG22 | 9.3-9.7 | -0.020 | 8.5-9.3 | ≥18 | -0.20 | 20-23 | 300 ℃ | 8.3 | |
XG24 | 9.5-10.2 | -0.025 | 8.7-9.6 | ≥18 | -0.20 | 22-24 | 300 ℃ | 8.3 | |
XG26 | 10.2-10.5 | -0.030 | 9.4-10.0 | ≥18 | -0.20 | 24-26 | 300 ℃ | 8.3 | |
XG28 | 10.3-10.8 | -0.035 | 9.5-10.2 | ≥18 | -0.20 | 26-28 | 300 ℃ | 8.3 | |
XG30 | 10.8-11.0 | -0.035 | 9.9-10.5 | ≥18 | -0.20 | 28-30 | 300 ℃ | 8.3 | |
XG32 | 11.0-11.3 | -0.035 | 10.2-10.8 | ≥18 | -0.20 | 29-32 | 300 ℃ | 8.3 | |
XG26M | 10.2-10.5 | -0.035 | 8.5-9.8 | 12-18 | -0.20 | 24-26 | 300 ℃ | 8.3 | |
XG28M | 10.3-10.8 | -0.035 | 8.5-10.0 | 12-18 | -0.20 | 26-28 | 300 ℃ | 8.3 | |
XG30M | 10.8-11.0 | -0.035 | 8.5-10.5 | 12-18 | -0.20 | 28-30 | 300 ℃ | 8.3 | |
XG32M | 11.0-11.3 | -0.035 | 8.5-10.7 | 12-18 | -0.20 | 29-32 | 300 ℃ | 8.3 | |
XG24L | 9.5-10.2 | -0.025 | 6.8-9.0 | 8-12 | -0.20 | 22-24 | 250 ℃ | 8.3 | |
XG26L | 10.2-10.5 | -0.035 | 6.8-9.4 | 8-12 | -0.20 | 24-26 | 250 ℃ | 8.3 | |
XG28L | 10.3-10.8 | -0.035 | 6.8-9.6 | 8-12 | -0.20 | 26-28 | 250 ℃ | 8.3 | |
XG30L | 10.8-11.5 | -0.035 | 6.8-10.0 | 8-12 | -0.20 | 28-30 | 250 ℃ | 8.3 | |
XG32L | 11.0-11.5 | -0.035 | 6.8-10.2 | 8-12 | -0.20 | 29-32 | 250 ℃ | 8.3 | |
Remak: · Nou rete menm jan ak pi wo a sof si espesifye nan kliyan an. Tanperati Curie ak koyefisyan tanperati yo se pou referans sèlman, pa kòm yon baz pou desizyon. · Tanperati maksimòm k ap travay nan leman se chanje akòz rapò nan longè ak dyamèt ak anviwònman faktè. |
Avantaj:
Sèvi ak leman sa yo kondisyone pa tanperati a nan yon pakèt domèn kouri soti nan 250ºC 350ºC ak tanperati Curie yo ka kòm yon wo
kòm 710 a 880 ° C. Se poutèt sa, SmCo leman gen pi bon estabilite mayetik akòz rezistans siperyè a tanperati ki wo.
Leman SmCo yo karakterize pa rezistans korozyon trè wo, pa gen okenn kouch ki nesesè pou pwoteksyon sifas yo.
Karakteristik:
Yon dezavantaj nan leman SmCo se frajilite ki make nan materyèl la - yon faktè ki dwe patikilyèman pran an kont pandan pwosesis la.
Leman yo galvanize oswa kouvwi pa electrodeposition katodik pou aplikasyon pou sèten.
Aplikasyon:
Nan zòn ki wo tanperati opere, segondè korozyon ak rezistans oksidasyon yo enpòtan anpil. Tankou, elektwonik magnetron,Magnetic transmisyon,
Mayetik tretman, Magnistor, elatriye.
Tout valè deklare yo te detèmine lè l sèvi avèk echantiyon estanda selon IEC 60404-5. Espesifikasyon sa yo sèvi kòm valè referans ak pouvwa
diferan. Maks la. tanperati opere depann sou dimansyon leman an ak aplikasyon espesifik la. Pou plis enfòmasyon tanpri kontakte nou
enjenyè aplikasyon yo.